Experimental dataset of highly flowable cementitious composites incorporating recycled tyre textile or polypropylene fibres: Central composite design and validation experiments
Description
This dataset presents raw and processed experimental data for 69 highly flowable cementitious composite mixtures incorporating either recycled tyre textile fibres (RTTF) or polypropylene fibres (PPF). The experimental programme comprises 64 mixtures developed using a central composite design (CCD), with 32 mixtures for each fibre type, and five additional validation mixtures (three RTTF and two PPF). Five mixture-design factors were investigated: water-to-cement ratio (w/c), water-to-powder volume ratio (Vw/Vp), sand-to-mortar volume ratio (Vs/Vm), fine-sand-to-total-sand volume ratio (Vsf/Vs), and fibre-to-powder volume ratio (Vf/Vp). Fibre type was considered at two categorical levels: RTTF and PPF. The dataset includes mixture compositions, coded design factors, fresh-state properties (D-flow diameter and V-funnel flow time), electrical resistivity measurements at 1, 7, 14 and 28 days, and mechanical properties (28-day flexural and compressive strengths). The accompanying Excel workbook contains the experimental measurements, processed mean values, a README sheet, a data dictionary, and coded-to-actual factor conversion information. These data support the analysis of mixture-design effects and provide a reference for developing and validating predictive models for fibre-reinforced cementitious composites.
Files
Steps to reproduce
The experimental dataset was generated using a five-factor central composite design (CCD) for highly flowable cementitious composites incorporating either recycled tyre textile fibres (RTTF) or polypropylene fibres (PPF). Experimental design: Define five mixture-design factors: water-to-cement ratio (w/c), water-to-powder volume ratio (Vw/Vp), sand-to-mortar volume ratio (Vs/Vm), fine-sand-to-total-sand volume ratio (Vsf/Vs), and fibre-to-powder volume ratio (Vf/Vp). Generate 32 experimental mixtures for each fibre type using the CCD, resulting in 64 design mixtures, and prepare five additional validation mixtures (three RTTF and two PPF). Mixture preparation: Calculate constituent quantities based on the experimental factor levels. Prepare each mixture using cement, limestone filler, fine and coarse sand, water, superplasticiser, and the designated fibre type. The coded factor levels, actual factor values, and mixture compositions are provided in the Excel dataset. Fresh-state testing: Measure the D-flow diameter and V-funnel flow time of the prepared mixtures and record the experimental results. Specimen preparation and curing: Cast three prismatic specimens measuring 40 × 40 × 160 mm for each mixture. Demould after approximately 24 hours and cure the specimens in water maintained at 20 ± 2 °C. Electrical resistivity testing: Measure electrical resistivity at 1, 7, 14 and 28 days and record the individual measurements and calculated mean values. Mechanical testing: At 28 days, perform flexural strength tests on the three prisms and compressive strength tests on the six resulting halves. Record the individual measurements and calculated mean strengths. Data processing: Organise the experimental measurements and calculated mean responses in the Excel workbook. Consult the README and Data Dictionary worksheets for variable definitions, measurement units, coded-to-actual factor conversion and interpretation of the dataset.
Institutions
- Universidade do PortoPorto, Porto
Categories
Funders
- Fundação para a Ciência e TecnologiaMinistry of Science Technology and Higher EducationLisbon, LisbonGrant ID: 2024.01063.BD