A polydimethylsiloxane dosage window for reduced water absorption and enhanced tensile strength in engineered geopolymer composites
Description
This dataset supports the study on pre-cured PDMS-modified fly ash–slag engineered geopolymer composites (EGC). The specimen series comprises one unmodified control (C-0) and six pre-cured PDMS dosages (PG-1 to PG-6, 1–6 wt% of binder mass), all containing 2 vol% PVA fibre. The dataset includes: (i) mass-based water absorption measured at 5, 10, 20, 30, 60 min and 2, 4, 8, 24, 48 and 72 h with three independent replicates per mix (specimens dried at 50 °C); (ii) direct tensile records, including the full representative 2000-point curves and the specimen-level peak stress and corresponding strain values; (iii) cube compressive strength at 3, 7 and 28 d and three-point flexural strength at 3, 7 and 28 d; (iv) contact angle values; (v) raw and processed FTIR spectra (KBr transmission) and raw XRD patterns; (vi) SEM image registration metadata and local EDS results; (vii) outputs of the statistical analyses (one-way ANOVA, Tukey HSD, Welch ANOVA and Games–Howell comparisons); and (viii) the Python scripts used to process the data, perform the statistical tests and generate the figures. Files are organised into raw data, processed data, figure source data, analysis scripts and supplementary source data. See README for a file-by-file description.
Files
Steps to reproduce
Mix design: Class I fly ash and S95 slag at 60:40 by mass, quartz sand at sand/binder = 0.20, activator of NaOH and sodium silicate (SiO2/Na2O = 2.0) prepared one day in advance, 2 vol% PVA fibre (12 mm, 39 micrometre), PDMS pre-mixed with TEOS and DBDL at 100:5:1 by mass and added in the final mixing step. Total mixing time 9 min. Water absorption: 40 mm cubes dried at 50 °C to constant mass, immersed with the water surface about 5 mm below the top face, weighed after wiping the surface at each time point. Wt = 100(Mt - M0)/M0, three independent replicates per mix. Mechanical tests: 70.7 mm cube compression at 0.5 MPa/s; 40x40x160 mm three-point flexure with 100 mm span at 50 N/s (GB/T 17671-2021); dog-bone direct tension at 0.1 mm/min crosshead displacement with a nominal 80 mm gauge length; three specimens per group and age. Microstructure: SEM on gold-coated fracture fragments at 10 kV; EDS normalised to the two listed elements; XRD over 4-70 degrees 2theta; FTIR by KBr transmission, 4 cm-1 nominal resolution, 32 scans, displayed over 500-4000 cm-1.
Institutions
- China University of Mining and TechnologyJiangsu, Xuzhou