Research data for: Coating and Doping Modification Strategies for Ni-rich Layered NCM Cathode Materials

Published: 7 October 2026| Version 1 | DOI: 10.17632/zn8jgrtxhv.1
Contributor:
Soumyadeep Ghosh

Description

This dataset contains the research data supporting the article "Coating and Doping Modification Strategies for Ni-rich Layered NCM Cathode Materials" (submitted to the Journal of Power Sources). LiNi0.9Co0.05Mn0.05O2 (NCM90) was modified with 1 and 2 mol% cerium through a solid-state reaction between a co-precipitated hydroxide precursor, LiOH·H2O and Ce(OH)3 (750 °C, 15 h, flowing O2). This gives a combined CeO2 surface coating with limited Ce incorporation. The dataset covers pristine NCM90, 1%-CeO2@NCM90 and 2%-CeO2@NCM90. Structural, morphological and surface-chemical data: powder XRD, SEM/EDS (including EDS maps after 100 cycles), HRTEM, and XPS (Ni 2p and Ce 3d spectra with fitted Ni3+ and Ce3+/Ce4+ fractions). Electrochemical data (CR2032 coin cells, Li-metal counter electrode, 1 M LiPF6 in EC:DEC, 2.7-4.3 V, 25 °C): galvanostatic charge-discharge and cycling at 1C over 200 cycles, rate capability (0.2-5C), cyclic voltammetry (0.1 mV/s), electrochemical impedance spectroscopy after 10 cycles, and dQ/dV analysis. Operando data: in situ XRD patterns recorded during the first two charge-discharge cycles. These data are qualitative, and lattice parameters were not refined.

Files

Steps to reproduce

1. Precursor synthesis (Ni0.9Co0.05Mn0.05(OH)2): Prepare 500 mL of a 2 mol/L transition-metal solution containing NiSO4·6H2O (236.6 g), CoSO4·7H2O (14.1 g) and MnSO4·H2O (8.5 g), giving Ni:Co:Mn = 90:5:5. Pump it at 0.1 mL/min into a 2 L stirred-tank reactor together with 4 mol/L NaOH and 4 mol/L NH3·H2O. Run at 50 °C under N2, stirring at 900 rpm. Hold the pH at 11.40 initially and then at 11.50 ± 0.05. 2. Precursor work-up: After feeding, stir the slurry for 72 h and age for 48 h at 400 rpm. Wash the precipitate with 0.6 mol/L ammonia solution and deionised water until the filtrate reaches pH 8. Dry at 60 °C for 24 h under vacuum. 3. Lithiation and Ce modification: Mix the precursor, LiOH·H2O and Ce(OH)3 at a molar ratio of 1 : 1.03 : 0.02 for 2%-CeO2@NCM90, or 1 : 1.03 : 0.01 for 1%-CeO2@NCM90. Calcine at 750 °C for 15 h in flowing O2 with a heating rate of 2 °C/min. Prepare pristine NCM90 the same way without Ce(OH)3. 4. Structural and surface characterisation: - XRD: Bruker D8 Discovery, Cu Kα, 10-80° 2θ. Index phases to the α-NaFeO2 structure (PDF#09-0063). - SEM/EDS: Zeiss Supra 55VP and EVO. - TEM: JEOL JEM-F200. - XPS: Record the Ni 2p and Ce 3d regions and fit the Ni3+ and Ce3+/Ce4+ fractions (Table 1 in the article). 5. Electrode preparation: Cast a slurry of active material, carbon black and PVDF (8:1:1 by weight) in N-methyl-2-pyrrolidone onto Al foil. Dry at 120 °C under vacuum overnight and roll-press. Active-material loading is about 4 mg/cm2. 6. Cell assembly: Assemble CR2032 coin cells in an Ar-filled glovebox (<0.1 ppm O2/H2O) with a Li-metal counter electrode, a Celgard 2400 separator and 1 mol/L LiPF6 in EC:DEC (1:1 by volume). 7. Electrochemical testing (25 °C, 2.7-4.3 V): - Galvanostatic charge-discharge: 1C for 200 cycles (initial curves; cycles 10-100 shown in the article). - Rate test: 0.2, 0.5, 1, 2 and 5C. - Cyclic voltammetry: 0.1 mV/s for the first five cycles. - EIS: after 10 cycles. Extract Rf and Rct from the Nyquist plots. - dQ/dV: calculate from the charge-discharge curves. 8. In situ XRD: Record XRD patterns during the first two charge-discharge cycles between 2.7 and 4.3 V. Follow the (104) reflection near 44.3° and the (101)/(012) and (018)/(110)/(113) regions. These data are qualitative, and lattice parameters were not refined. 9. Post-cycling analysis: After 100 cycles at 1C, collect EDS maps of 2%-CeO2@NCM90 to check the Ce distribution.

Categories

Cathode Materials for Batteries, Lithium Ion Battery, Battery Energy Storage